摘要
通过强化孕育,细化石墨球,减轻锰的偏析,以Mn-Cu或Mn-Cr作为合金元素,获得铸态混合型基体组织。可得到σb>600MPa或>550MPa,同时具有σ>10%的高性能。
Mixed matrix structure was obtained by intensifying inoculation of increasing the S.G. count,reducing the segregation of Mn,and simultaneously, by adapting definite content of copper or chrominum whichtogather with manganese acted as strenthening elements. As a results the high ductile and properties,σb>600MPa or>550MPa and σ>10%,were reached.
出处
《铸造技术》
CAS
北大核心
1995年第2期41-43,共3页
Foundry Technology
关键词
偏析
孕育处理
合金化
球墨铸铁
铸造
Strenghthaning inorulation Segregation Mixed matrix