摘要
原矿的多元素分析和铜铅矿物的物相分析结果表明,该矿石以黄铜矿和方铅矿为主,其氧化率分别为25.8%、28.88%。通过"铜铅混浮、尾矿选锌、铜铅分离"的工艺流程,调整剂用"重铬酸钾+亚硫酸钠"作组合抑铅浮选铜,顺利实现了混合铜铅精矿的分离。
This article is based on multi-elements, analysis copper phase and lead phase, The ore is main made of chalcoprite with the oxidation rate 25.8% and galena with the oxidation rate 28.88%. Adopt the process as follow, mix-flotation of copper and lead, separation of the concentrate of lead and copper, zinc flotation from tail, Use sodium sulfite+ dichromate as the adjusting agent to contain lead, the bulk lead-copper concentration were separated.
出处
《中国矿业》
北大核心
2007年第10期74-76,共3页
China Mining Magazine
关键词
混合浮选
组合抑制剂
铜铅分离
bulk flotation
combined depressen
copper-lead separation