摘要
以乙酸钯为前体、三缩四乙二醇为溶剂和还原剂,在不使用保护剂、适量无水乙酸钠存在下,60℃水浴加热4 min,乙酸钯还原得到溶剂稳定的粒径小、大小均一、分散性好的钯纳米颗粒,平均粒径为(3.51±0.49)nm。
Solvent-stabilized Pd nanoparticles with a small diameter, uniform size and good dispersion were synthesized by reducing palladium acetate with tetraethylene glycol as both a solvent and a reducing agent in the presence of an appropriate amount of anhydrous sodium acetate without using any special protecting agent under water-bath heating at 60℃ for 4 min. The mean size of the as-prepared Pd nanoparticles was(3.51±0.49) nm.
出处
《化学与生物工程》
CAS
2010年第1期13-15,18,共4页
Chemistry & Bioengineering
基金
国家自然科学基金资助项目(20673146)
中南民族大学重点基金资助项目(YZZ05002)
关键词
钯
乙酸钯
乙酸钠
纳米颗粒
三缩四乙二醇
palladium
palladium acetate
sodium acetate
nanoparticle
tetraethylene glycol