摘要
通过设备改造和工艺调整,增加零罗拉,选择加工速度550~600 m/min,D/Y比1.68~1.70,拉伸倍数1.68~1.72,第二热箱温度120~140℃,网络压力达到0.23 MPa以上等工艺条件时,生产出性能优良的涤纶复合丝。
By innovating equipment and adjusting process parameters, the POY and DTY polyester composite filament can be produced with excellent properties, through the addition of zero roller, under the conditions as follows : texturizing machine speed 550 - 600 m/rain, D/Y ratio of 1.68 - 1.70, draw ratio of 1.68 - 1.72, the second heater temperature 120 - 140 ℃ and intermingling press above 0.23 Mpa.
出处
《化纤与纺织技术》
2013年第1期4-6,共3页
Chemical Fiber & Textile Technology
关键词
复合丝
工艺
设备改造
网络
composite filament
process
equipment innovation
intermingling