The stability of underground abandoned gypsum mines is dependent on the gypsum pillar's strength,and most abandoned mines are in a fully saturated condition. Moisture affects the strength of gypsum and is therefor...The stability of underground abandoned gypsum mines is dependent on the gypsum pillar's strength,and most abandoned mines are in a fully saturated condition. Moisture affects the strength of gypsum and is therefore commonly measured when testing rock strength. For most rocks, this is a simple task of weighing the rock's mass before and after oven-heating at a specified temperature and duration. For natural gypsum, however, this is not a straightforward process. Heating natural gypsum can result in dehydration and transformation of gypsum to hemihydrate and anhydrite, thus changing the physical characteristics of the gypsum such as its particle density which in turn affects the moisture content and strength measurements. To prevent transformation when determining the moisture content of gypsum,the American Society for Testing Materials(ASTM) recommends lowering the drying temperature from 110℃ to 60℃ . To investigate the temperature at which gypsum transforms to hemihydrate, we used a helium pycnometer to measure the particle densities of gypsum, hemihydrate and anhydrite. In this research, we suggest that a higher drying temperature of 80℃ can be used for drying gypsum without transforming gypsum to hemihydrate. Further, preparing saturated samples for mechanical testing,which is required in stability analyses of abandoned mines, is challenging due to the dissolution of gypsum when placed in water. To address this problem, we investigated the following methods to saturate gypsum cores taking into account the solubility of gypsum:(1) water immersion,(2) vacuum saturation, and(3) improved vacuum saturation. The research indicates that all the three methods are acceptable but they should be conducted using a saturated gypsum-water solution to minimize dissolution. Further, the research found that the improved vacuum saturation method saturated the test samples within 24 h, while duration of 30 h was required for the other two methods.展开更多
Density and porosity are fundamental and important physical properties of rocks in various geological problems, and affect the other physical properties. Therefore, measurements of density and porosity of rock samples...Density and porosity are fundamental and important physical properties of rocks in various geological problems, and affect the other physical properties. Therefore, measurements of density and porosity of rock samples are important investigation items in both geo-science and geo-engineering areas. Several measurement techniques of the density and porosity are available and being applied currently. To ensure the data quality and to conduct its quality assessment, comparison of measurement results by different measurement techniques is necessary since the techniques are based on different principles and test procedures. In this study, we collected eight types of rock samples including a gabbro, a granite, four sandstones, a welded tuff and a mudstone as study materials, and also prepared several metal specimens for the experimental comparison. The porosities of the eight rocks covered a very wide range from 0.3% to 50% approximately. We employed three methods (caliper, buoyancy and helium-displacement pycnometer) to measure volumes of regularly-shaped specimens and to determine their bulk densities and porosities. As a result, the three techniques yielded almost same bulk densities and porosities for all the specimens. In addition, we also applied mercury intrusion porosimetry to measure density and porosity as well as to determine pore size distribution of the rock samples. Porosity values obtained by the porosimetry method were underestimated in the case of high-porosity (soft) rock samples and overestimated for the very low-porosity rock samples. Ability to determine pore size distribution, however, is a very important advantage of the porosimetry method.展开更多
The amount of fine material available in the soil is significant in Atterberg limits and methylene blue tests. In the context of Atterberg limits, increased amount of clay minerals contained in the soil increases liqu...The amount of fine material available in the soil is significant in Atterberg limits and methylene blue tests. In the context of Atterberg limits, increased amount of clay minerals contained in the soil increases liquid and plastic limit values;however, increasing sand content reduces the moisture content reducing the water retention capacity of the soil which in return reduces the plasticity index (PI) value. In the case of methylene blue test, which is used to specify the quality of the amount of fine material, existence of clay in the medium increases the pollution level of the sand and the amount of methylene solution (V1) used. In this study, soil classes were determined and pollution rates were identified with Atterberg limits, pycnometer, sieve analysis, hydrometer analysis and methylene blue tests conducted on 11 different natural soil samples collected from different regions. From the data obtained, first the relationship between PI and methylene blue (MB) was examined and was evaluated according to the results of the “single regression” method. Furthermore, the other coefficient of uniformity (Cu), coefficient of graduation (Cc), unit weight of soils (γs) parameters obtained from experimental studies were also subjected to “multiple regression analysis” in order to reveal their impact on the MB and this impact was confirmed taking both statistical analyses into account.展开更多
文摘The stability of underground abandoned gypsum mines is dependent on the gypsum pillar's strength,and most abandoned mines are in a fully saturated condition. Moisture affects the strength of gypsum and is therefore commonly measured when testing rock strength. For most rocks, this is a simple task of weighing the rock's mass before and after oven-heating at a specified temperature and duration. For natural gypsum, however, this is not a straightforward process. Heating natural gypsum can result in dehydration and transformation of gypsum to hemihydrate and anhydrite, thus changing the physical characteristics of the gypsum such as its particle density which in turn affects the moisture content and strength measurements. To prevent transformation when determining the moisture content of gypsum,the American Society for Testing Materials(ASTM) recommends lowering the drying temperature from 110℃ to 60℃ . To investigate the temperature at which gypsum transforms to hemihydrate, we used a helium pycnometer to measure the particle densities of gypsum, hemihydrate and anhydrite. In this research, we suggest that a higher drying temperature of 80℃ can be used for drying gypsum without transforming gypsum to hemihydrate. Further, preparing saturated samples for mechanical testing,which is required in stability analyses of abandoned mines, is challenging due to the dissolution of gypsum when placed in water. To address this problem, we investigated the following methods to saturate gypsum cores taking into account the solubility of gypsum:(1) water immersion,(2) vacuum saturation, and(3) improved vacuum saturation. The research indicates that all the three methods are acceptable but they should be conducted using a saturated gypsum-water solution to minimize dissolution. Further, the research found that the improved vacuum saturation method saturated the test samples within 24 h, while duration of 30 h was required for the other two methods.
文摘Density and porosity are fundamental and important physical properties of rocks in various geological problems, and affect the other physical properties. Therefore, measurements of density and porosity of rock samples are important investigation items in both geo-science and geo-engineering areas. Several measurement techniques of the density and porosity are available and being applied currently. To ensure the data quality and to conduct its quality assessment, comparison of measurement results by different measurement techniques is necessary since the techniques are based on different principles and test procedures. In this study, we collected eight types of rock samples including a gabbro, a granite, four sandstones, a welded tuff and a mudstone as study materials, and also prepared several metal specimens for the experimental comparison. The porosities of the eight rocks covered a very wide range from 0.3% to 50% approximately. We employed three methods (caliper, buoyancy and helium-displacement pycnometer) to measure volumes of regularly-shaped specimens and to determine their bulk densities and porosities. As a result, the three techniques yielded almost same bulk densities and porosities for all the specimens. In addition, we also applied mercury intrusion porosimetry to measure density and porosity as well as to determine pore size distribution of the rock samples. Porosity values obtained by the porosimetry method were underestimated in the case of high-porosity (soft) rock samples and overestimated for the very low-porosity rock samples. Ability to determine pore size distribution, however, is a very important advantage of the porosimetry method.
文摘The amount of fine material available in the soil is significant in Atterberg limits and methylene blue tests. In the context of Atterberg limits, increased amount of clay minerals contained in the soil increases liquid and plastic limit values;however, increasing sand content reduces the moisture content reducing the water retention capacity of the soil which in return reduces the plasticity index (PI) value. In the case of methylene blue test, which is used to specify the quality of the amount of fine material, existence of clay in the medium increases the pollution level of the sand and the amount of methylene solution (V1) used. In this study, soil classes were determined and pollution rates were identified with Atterberg limits, pycnometer, sieve analysis, hydrometer analysis and methylene blue tests conducted on 11 different natural soil samples collected from different regions. From the data obtained, first the relationship between PI and methylene blue (MB) was examined and was evaluated according to the results of the “single regression” method. Furthermore, the other coefficient of uniformity (Cu), coefficient of graduation (Cc), unit weight of soils (γs) parameters obtained from experimental studies were also subjected to “multiple regression analysis” in order to reveal their impact on the MB and this impact was confirmed taking both statistical analyses into account.