High-alkali species in coal are notorious for causing ash slagging and fouling incidents.In this paper,four high-alkali coals were individually subject to hydrothermal pretreatment(HTP),within a batch-type autoclave a...High-alkali species in coal are notorious for causing ash slagging and fouling incidents.In this paper,four high-alkali coals were individually subject to hydrothermal pretreatment(HTP),within a batch-type autoclave at 300 -C for 1 h,and the treated coals were analyzed,along with the oxygen-containing functional groups determined by Fourier transform infrared spectrometer(FT-IR).Then the alkali species and other components in the coal ash were quantified by X-ray fluorescence(XRF)for evaluating the ash slagging and fouling tendency.Apart from this,FactSage was adopted to simulate the occurrence and transformation of alkali species during coal thermal conversion ending at various temperatures.The findings indicate that the treated coals are superior to the parent ones in terms of certain remarkable changes via HTP.The moisture,oxygen and sulfur of the hydrothermally treated coals decline obviously,while the calorific value rises sharply.HTP could reduce the alkali species to less than 2%(%,by weight,equivalent to Na2O in dry ash),with a maximum removal ratio of 88.9%,lowering the ash slagging and fouling tendency.The proposed mechanism of HTP was that the alkali species in coal matrix became released due to the breakage of the coal functional groups and micropores during HTP.展开更多
The migration characteristics of heavy metals in co-combustion of sewage sludge and high alkali coal in circulating fluidized bed were studied by experiments and simulations. Temperature plays a crucial role in thermo...The migration characteristics of heavy metals in co-combustion of sewage sludge and high alkali coal in circulating fluidized bed were studied by experiments and simulations. Temperature plays a crucial role in thermodynamic equilibrium distribution and migration characteristics of heavy metals. At the temperature range of 700℃-1200℃, Hg is completely gaseous and the proportion of Pb, Ni, and Cd in the gas phase is also high. As is mainly elemental in the system, and the proportion of Cr in the solid phase is large. Zn compounds are diverse and mostly solid materials. The volatility of Cu is not strong, and it will become gaseous when the temperature exceeds 1700℃. The proportion of heavy metals in the gas phase decreases as the excess air ratio increases. In an oxygen-rich atmosphere, most of Zn and Ni are converted to oxides;Pb and Cd are converted to crystalline silicate;Cu is converted to partial aluminate;Cr compound is decomposed to form Cr_(2)O_(3);they are good for the solidification and controlling of heavy metals. The elemental Hg is converted to HgCl_(2) and the elemental As is converted to AsCl_(3). Temperature also has a great influence on the volatilization rate of heavy metals. The higher the temperature, the shorter the time they reach the maximum volatility.展开更多
基金the National Key Basic Research Program of China (No. 2014CB238905)
文摘High-alkali species in coal are notorious for causing ash slagging and fouling incidents.In this paper,four high-alkali coals were individually subject to hydrothermal pretreatment(HTP),within a batch-type autoclave at 300 -C for 1 h,and the treated coals were analyzed,along with the oxygen-containing functional groups determined by Fourier transform infrared spectrometer(FT-IR).Then the alkali species and other components in the coal ash were quantified by X-ray fluorescence(XRF)for evaluating the ash slagging and fouling tendency.Apart from this,FactSage was adopted to simulate the occurrence and transformation of alkali species during coal thermal conversion ending at various temperatures.The findings indicate that the treated coals are superior to the parent ones in terms of certain remarkable changes via HTP.The moisture,oxygen and sulfur of the hydrothermally treated coals decline obviously,while the calorific value rises sharply.HTP could reduce the alkali species to less than 2%(%,by weight,equivalent to Na2O in dry ash),with a maximum removal ratio of 88.9%,lowering the ash slagging and fouling tendency.The proposed mechanism of HTP was that the alkali species in coal matrix became released due to the breakage of the coal functional groups and micropores during HTP.
基金supported by the National Natural Science Foundation of China(No.52076172)。
文摘The migration characteristics of heavy metals in co-combustion of sewage sludge and high alkali coal in circulating fluidized bed were studied by experiments and simulations. Temperature plays a crucial role in thermodynamic equilibrium distribution and migration characteristics of heavy metals. At the temperature range of 700℃-1200℃, Hg is completely gaseous and the proportion of Pb, Ni, and Cd in the gas phase is also high. As is mainly elemental in the system, and the proportion of Cr in the solid phase is large. Zn compounds are diverse and mostly solid materials. The volatility of Cu is not strong, and it will become gaseous when the temperature exceeds 1700℃. The proportion of heavy metals in the gas phase decreases as the excess air ratio increases. In an oxygen-rich atmosphere, most of Zn and Ni are converted to oxides;Pb and Cd are converted to crystalline silicate;Cu is converted to partial aluminate;Cr compound is decomposed to form Cr_(2)O_(3);they are good for the solidification and controlling of heavy metals. The elemental Hg is converted to HgCl_(2) and the elemental As is converted to AsCl_(3). Temperature also has a great influence on the volatilization rate of heavy metals. The higher the temperature, the shorter the time they reach the maximum volatility.